熊娟,郑兴文,张文艳,范金龙,黄恩龙.西南地区某输油管道外腐蚀分析[J].表面技术,2014,43(4):59-63,157.
XIONG Juan,ZHENG Xing-wen,ZHANG Wen-yan,FAN Jin-long,HUANG En-long.Analysis on the External Corrosion for an Oil Pipeline in Southwest China[J].Surface Technology,2014,43(4):59-63,157
西南地区某输油管道外腐蚀分析
Analysis on the External Corrosion for an Oil Pipeline in Southwest China
投稿时间:2014-04-03  修订日期:2014-06-10
DOI:
中文关键词:  输油管道  外腐蚀  土壤  腐蚀产物  腐蚀机理
英文关键词:oil pipeline  external corrosion  soil  corrosion products  corrosion mechanism
基金项目:
作者单位
熊娟 西南油气田分公司 输气管理处, 成都 610500 
郑兴文 四川理工学院 化学与制药工程学院, 四川 自贡 643000;材料腐蚀与防护四川省重点实验室,四川 自贡 643000 
张文艳 西南油气田分公司 输气管理处, 成都 610500 
范金龙 材料腐蚀与防护四川省重点实验室,四川 自贡 643000 
黄恩龙 材料腐蚀与防护四川省重点实验室,四川 自贡 643000 
AuthorInstitution
XIONG Juan Gas Transmission Management Department, Petro China Southwest Oil and Gas Field Company, Chengdu 610500, China 
ZHENG Xing-wen School of Chemical and Pharmaceutical Engineering, Sichuan University of Science & Engineering, Zigong 643000, China;Key Laboratory of Material Corrosion and Protection of Sichuan Province, Zigong 643000, China 
ZHANG Wen-yan Gas Transmission Management Department, Petro China Southwest Oil and Gas Field Company, Chengdu 610500, China 
FAN Jin-long Key Laboratory of Material Corrosion and Protection of Sichuan Province, Zigong 643000, China 
HUANG En-long Key Laboratory of Material Corrosion and Protection of Sichuan Province, Zigong 643000, China 
摘要点击次数:
全文下载次数:
中文摘要:
      目的 研究西南地区某输油管道外腐蚀行为。 方法 现场检测,对土壤理化性质及腐蚀产物成分进行室内分析。 结果 开挖点 A 的土壤呈弱碱性,土壤腐蚀性弱,管道发生轻微均匀腐蚀,腐蚀产物主要为 FeO( OH) ,Fe( OH)3 和 Fe3O4 等铁的氧化物,对应的阴极反应为吸氧反应;开挖点 B 的土壤酸性强,硫酸根离子浓度高,土壤腐蚀性强,管道发生严重坑蚀,腐蚀产物主要成分为 FeSO4 ·7 H2O 及少量碱式硫酸铁,对应的阴极反应以析氢反应为主。 结论 开挖点土壤的理化性质差异,导致管道的腐蚀形态、腐蚀产物和腐蚀机理显著不同。
英文摘要:
      Objective To investigate the external corrosion for two excavation points of an oil pipeline in southwest China. Methods Through the on-site testing and laboratory analysis on phys-chemical properties of soil and composition of corrosion product. Results The soil is slightly basic for the excavation point A, and its corrosivity is weak, as a result, where the pipeline suffer weakly uniform corrosion, and the corrosion products are mainly iron oxides, including FeO( OH) , Fe( OH)3 and Fe3 O4 , also the cathodic reaction is reduction of dissolved oxygen. While for excavation point B, because of the strong acidity and high content of sulfate ion, the soil is highly corrosive and makes the pipeline suffer serious pitting corrosion, and corrosion products are mainly composed by FeSO4 ·7H2 O, also contains a small amount of basic ferric sulfate, moreover the cathodic process is mainly the reduction of hydrogen ions. Conclusion Due to the significant difference of the phys-chemical properties of soil, there are notably different on the corrosion morphology, products and mechanism of pipeline between two excavation points.
查看全文  查看/发表评论  下载PDF阅读器
关闭

关于我们 | 联系我们 | 投诉建议 | 隐私保护 | 用户协议

您是第24187378位访问者    渝ICP备15012534号-3

版权所有:《表面技术》编辑部 2014 surface-techj.com, All Rights Reserved

邮编:400039 电话:023-68792193传真:023-68792396 Email: bmjs@surface-techj.com

渝公网安备 50010702501715号